Physical properties of Saran™ Fibers

1.Tensile Strength
1.3~2.0 cN/dtex (1.4~2.2 g/d) (at room temperature)
2.Tensile Elongation
20%~40% (at room temperature)
3.Knot Strength
0.89~1.4 cN/dtex (1.0~1.6g/d ) 
4.Knot Elongation
10~12%
5.Young's Modulus
1.2~1.8 GPa (120~180kg/mm²)
6.Elastic Recovery
over 95% (at 3% elongation)
7.Specific Gravity
1.7
8.Moisture Regain
below 0.1%
9.Melting point
approximately 160ºC

Chemical resistance of Saran™

90-day immersion at room temperature

Agent Strength Deterioration
after 90days
Coloration
Hydrochloric acid 10% 0 none
20% 0 none
35% 0 Tinge of yellow
Sulfuric acid 20% 0 none
50% 10% none
95% 20% Blackish brown after two months
Nitric acid 10% 0 none
20% 0 Light yellow
50% 0 Light yellowish green
Sodium hydroxide 10% 0 none
20% 0 Yellow
50% 0 Yellow
Potassium hydroxide 10% 0 none
20% 0 Dark brown
50% 0 Dark brown
Aqueous ammonia 1% 0 Yellow
5% 10% Deep brown
10% 20% Blackish brown
Potassium permanganate 3% 0 Blackish brown
Bleach 3% 0 Blackish brown
Bromine water 3% 0 Blackish brown
Alcohol   0 Light yellow
Aceton   10% Yellow
Ether   50% Black Color
Calcic water 6% 0 Yellow
Carbon bisulfide   10% Yellow
Aniline   10% Blackish brown
Petroleum ether   0 Yellow
Glacial acetic acid   0 Light yellow

< Previous Page: Features

ASAHI KASEI HOME PRODUCTS
PVDC fiber " Saran™ "
Saran™
- Features of PVDC fiber " Saran™ "
- Physical properties
Fiber Line Up
- Doll Hair
- BioContactor for Wastewater treatment
- PVDC Fiber(Saran™) Line Up
Saran™ Applications INDEX
- SARAN SCREEN™/SARAN HONEYCOMB™
- Wet filter
- SARAN LOCK™
- Blind
- Other Applications
Contact Us